AWS A5.23: Mea Hoʻolako Mea Hoʻopau Uea Hoʻoheheʻe Arc Submerged ECM4

Wehewehe Pōkole:

AWS A5.23: ʻO ka ECM4 Submerged Arc Solid Wire kahi electrode uea i hoʻohui ʻia me ka metala haʻahaʻa no ka hoʻoheheʻe ʻana i ka arc i lalo i nā noi ikaika kiʻekiʻe. AWS A5.23: Ua hui ʻo ECM4 me ka kemika AWS A5.23 M4, a ua hoʻolālā ʻia no nā pae ikaika tensile ma luna o 110 ksi.


Nā kikoʻī huahana

Nā Lepili Huahana

WEHEWEHE:

Nā Uea ʻAla i Hoʻokomo ʻia i loko o ka Wai Hoʻoheheʻe ʻia nā Kila Haʻahaʻa

MĀHELE:

AWS A5.23: ʻO ka ECM4 Submerged Arc Solid Wire kahi electrode uea i hoʻohui ʻia me ka metala haʻahaʻa no ka hoʻoheheʻe ʻana i ka arc i lalo i nā noi ikaika kiʻekiʻe. AWS A5.23: Ua hui ʻo ECM4 me ka kemika AWS A5.23 M4, a ua hoʻolālā ʻia no nā pae ikaika tensile ma luna o 110 ksi.

KA PALAPALA NUI:

Nā noi hele hoʻokahi a me nā noi he nui me ka flux arc submerged i ʻōlelo ʻia, nā kila Low-Alloy ikaika kiʻekiʻe, nā kila Quench & Tempered, nā ʻāpana lako kaumaha, nā ʻāpana kūkulu, nā ʻili moku, nā kila i hoʻolei ʻia, nā ipu paila a me nā moku kaomi

Nā kila HSLA a me Q&T

Hana ʻana i ke ʻano kūkulu

Ka hana ʻana o ka Jack-up rig

Nā mōlina lako kaumaha

Nā kaola crane

NĀ HIʻONA:

Hiki i ke kaula hao-cored ke hāʻawi i nā helu hoʻokaʻawale i hoʻomaikaʻi ʻia i hoʻohālikelike ʻia me nā kaula paʻa i nā amperages like

Hāʻawi nā uea metala-core i nā ʻano komo ākea i hoʻohālikelike ʻia me nā uea paʻa ma nā ʻano hoʻohālikelike hoʻohui

Waihona ikaika kiʻekiʻe loa me ka paʻakikī haʻahaʻa haʻahaʻa maikaʻi loa i ke kūlana i hoʻopaʻa ʻia

Ua like nā koi kemika waiho weld me nā koi o nā uea paʻa EM4.

Nā Hoʻokaʻawale ʻana o AWS:

Me ke kahe Kūlana Nā kikoʻī Hoʻokaʻawale ʻana (Nā ʻĀpana Maʻamau o ʻAmelika Hui Pū ʻIa) Hoʻokaʻawale ʻana (Nā ʻĀpana SI)
SWX 150 Hoʻopili ʻia e like me ke kuʻi ʻia A5. 23/A5 23M F11A10-ECM4-M4 F76A7-ECM4-M4
Me ke kahe %C % Mn %Si %P %S % Cu % Cr % Ni % Mo %TI+V+Zr
SWX 150 0.06 1.45 0.27 0.012 0.010 0.06 0.31 2.25 0.47 0.02

KA HOʻOHUI KEMIKALA MAʻAMAU O KE WEHE:

Me ke kahe Hydrogen Hoʻolaha
SWX 150 7.5 ml/100g

NĀ ʻANO MEKANI MAʻAMAU:

Me ke kahe Kūlana Ikaika Hoʻopaʻa Ikaika Hāʻawi % Elongation ma 2" (50 mm)
SWX 150 Hoʻopili ʻia e like me ke kuʻi ʻia 113 ksi (779 MPa) 106 ksi (731 MPa) 20%
PWHT* 104 ksi (717 MPa) 97 ksi (669 MPa) 8%

Nā Waiwai Hopena Maʻamau o CHARPY V-NOTCH:

Me ke kahe Kūlana ʻAwelike ma -60°F (-50°C) ʻAwelike ma -80°F (-60°C) ʻAwelike ma -100°F (-70°C)
SWX 150 Hoʻopili ʻia e like me ke kuʻi ʻia 55 kapuaʻi-lbs (75 J) 60 f-bs (81 J) 45 f-ʻIwi (61 J)
PWHT* 57 f-lbs (77 J) 45 kapuaʻi-lbs (61 J) —

NĀ KUMU HANA MAʻAMAU:

vsvsv


  • Ma mua:
  • Aʻe: